Green Sand Castings are castings made using wet sand or “green sand” molds. The sand is not green in color nor do the molds use “greensand,” a greenish color sandstone. Instead of the sand is called “green” because it has moisture in it (like green wood) before the sand dries out when molten metal is poured in the mold.
What gives the sand moisture and helps the sand stick together when making molds is the clay that is mixed in the sand. Bentonite clay and the sand mixed together provide strong molds that can be created on an automated assembly line.
Sinteraður keramiksteypusandur er aðallega gerður úr steinefnum sem innihalda Al2O3 og SiO2 og bætt við öðrum steinefnum. Kúlulaga steypusandur framleiddur með duft-, kögglunar-, sintunar- og flokkunarferlum. Helsta kristalbygging þess er Mullite og Corundum, með ávöl kornform, hár eldfastur, góður hitaefnafræðilegur stöðugleiki, lítill varmaþensla, högg- og slitþol, eiginleikar sterkra sundrungar. Þegar keramiksandurinn er notaður í grænan sandferli, gæti það aukið endurnýtingartíma hrásands, dregið úr losun úrgangssandi, bætt steypuafrakstur.
● Ofurháhitaþol og framúrskarandi öndun gera háan vélrænan endurheimtahraða sandi, lægri losun úrgangssandi.
● Mikil gegndræpi. Gegndræpi græna sandsins sem blandaður var með hertu keramiksteypusandi var meiri en blönduð kvarssandi við sömu vinnsluaðstæður.
Kornastærðardreifinguna er hægt að aðlaga í samræmi við kröfur þínar.
Möskva |
20 | 30 | 40 | 50 | 70 | 100 | 140 | 200 | 270 | Pan | AFS | |
μm |
850 | 600 | 425 | 300 | 212 | 150 | 106 | 75 | 53 | Pan | ||
kóða | 40/70 | ≤5 | 20-30 | 40-50 | 15-25 | ≤8 | ≤1 | 43±3 | ||||
70/40 | ≤5 | 15-25 | 40-50 | 20-30 | ≤10 | ≤2 | 46±3 | |||||
50/100 | ≤5 | 25-35 | 35-50 | 15-25 | ≤6 | ≤1 | 50±3 | |||||
100/50 | ≤5 | 15-25 | 35-50 | 25-35 | ≤10 | ≤1 | 55±3 | |||||
70/140 | ≤5 | 25-35 | 35-50 | 8-15 | ≤5 | ≤1 | 65±4 |